Propertya | Test Methodb | Typical Value, Unitsc |
|
Electrical Properties |
Dielectric Constant | |
1 kHz | D 150 | 2.6 |
1 MHz | D 150 | 2.4 |
Dissipation Factor | | 1 kHz | D 150 | 0.005 |
1 MHz | D 150 | 0.02 |
Arc Resistance | D 495 | 158 sec |
Volume Resistivity | D 257 | 1015 ohm·cm |
Surface Resistivity | D 257 | 1016 ohms/square |
Dielectric Strength, Short Time, 500 V/sec rate-of-rise | D 149 | 16 kV/mm (410 V/mil) |
Film Properties |
|
Thickness of Film Tested | D 374 | 250 Microns (10 mils) |
Density | D 1505 | 1.27 g/cm3 |
Haze | D 1003 | 0.8 % |
Gloss | | @ 45° | D 2457 | 108 |
Transparency | D 1746 | 85 % |
Regular Transmittance | D 1003 Modified | 89 % |
Total Transmittance | D 1003 Modified | 91 % |
Water Vapor Transmission Ratee | F 1249 | 7 g/m2·24h (0.5 g/100in.2·24h) |
Gas Permeability, CO2 | D 1434 | 49 cm3·mm/m2·24h·atm (125 cm3·mil/100in.2·24h·atm) |
Gas Permeability, O2 | D 3985 | 10 cm3·mm/m2·24h·atm (25 cm3·mil/100in.2·24h·atm) |
Elmendorf Tear Resistance | | M.D. | D 1922 | 13.7 N (1400 gf) |
T.D. | D 1922 | 16.7 N (1700 gf) |
PPT Tear Resistance | | M.D. | D 2582 | 93 N (21 lbf) |
T.D. | D 2582 | 93 N (21 lbf) |
Tear Propagation Resistance, Split Tear Method | | @ 254 mm/min (10 in./min) M.D. | D 1938 | 36 N/mm (205 lbf/in.) |
@ 254 mm/min (10 in./min) T.D. | D 1938 | 36 N/mm (205 lbf/in.) |
Tear Resistance, Trouser @ 200 mm/min | | M.D. | ISO 6383-1 | 36 N/mm (205 lbf/in.) |
T.D. | ISO 6383-1 | 36 N/mm (205 lbf/in.) |
Tensile Strength @ Yield | | M.D. | D 882 | 52 MPa (7500 psi) |
T.D. | D 882 | 52 MPa (7500 psi) |
Tensile Strength @ Break | | M.D. | D 882 | 59 MPa (8600 psi) |
T.D. | D 882 | 55 MPa (8000 psi) |
Elongation @ Yield | | M.D. | D 882 | 4 % |
T.D. | D 882 | 4 % |
Elongation @ Break | | M.D. | D 882 | 400 % |
T.D. | D 882 | 400 % |
Tensile Modulus | | M.D. | D 882 | 1300 MPa (1.9 x 105 psi) |
T.D. | D 882 | 1300 MPa (1.9 x 105 psi) |
Dart Impacti | | @ -18°C (0°F) | D 1709A Modified | 500 g |
@ 23°C (73°F) | D 1709A Modified | 400 g |
Mechanical Properties (Injection Molded), ASTM Method |
|
Specific Gravity | D 792 | 1.27 |
Water Absorption, 24 h immersion | D 570 | 0.13 % |
Tensile Stress @ Break | D 638 | 28 MPa (4100 psi) |
Tensile Stress @ Yield | D 638 | 50 MPa (7300 psi) |
Elongation @ Break | D 638 | 130 % |
Tensile Modulus | D 638 | 2100 MPa (3.0 x 105 psi) |
Flexural Modulus | D 790 | 2100 MPa (3.0 x 105 psi) |
Flexural Yield Strength | D 790 | 70 MPa (10200 psi) |
Rockwell Hardness, R Scale | D 785 | 106 |
Izod Impact Strength, Notched | | @ 23°C (73°F) | D 256 | 101 J/m (1.9 ft·lbf/in.) |
@ -40°C (-40°F) | D 256 | 37 J/m (0.7 ft·lbf/in.) |
Impact Strength, Unnotchedg | | @ -20°C (-4°F) | D 4812 | NB |
@ 23°C (73°F) | D 4812 | NB |
@ -30°C (-22°F) | D 4812 | NB |
@ -40°C (-40°F) | D 4812 | NB |
Impact Resistance (Puncture), Energy @ Max. Load | | 2.5-mm (0.100-in.) Thick Plaques, @ 23°C (73°F) | D 3763 | 28 J (21 ft·lbf) |
2.5-mm (0.100-in.) Thick Plaques, @ -40°C (-40°F) | D 3763 | 41 J (30 ft·lbf) |
3.2-mm (0.125-in.) Thick Plaques @ 23°C (73°F) | D 3763 | 33 J (24 ft·lbf) |
3.2-mm (0.125-in.) Thick Plaques @ -40°C (-40°F) | D 3763 | 50 J (37 ft·lbf) |
Mechanical Properties (Injection Molded), ISO Method |
|
Density | ISO 1183, Method D | 1.27 g/cm3 |
Water Absorption, 24 h immersion | ISO 62 | 0.13 % |
Tensile Stress @ Break | ISO 527 | 28 MPa |
Tensile Stress @ Yield | ISO 527 | 50 MPa |
Elongation @ Break | ISO 527 | 100 % |
Tensile Modulus | ISO 527 | 2100 MPa |
Flexural Modulus | ISO 178 | 2000 MPa |
Flexural Yield Strength | ISO 178 | 68 MPa |
Rockwell Hardness, R Scale | ISO 2039-2 | 109 |
Izod Impact Strength, Notched, Type 1 Specimen, Type A Notch | | @ 23°C | ISO 180 | 6.2 kJ/m2 |
@ -40°C | ISO 180 | 4.2 kJ/m2 |
Impact Strength, Unnotched, Type 1 Specimenf | | @ -20°C | ISO 180 | NB kJ/m2 |
@ 23°C | ISO 180 | NB kJ/m2 |
@ -30°C | ISO 180 | NB kJ/m2 |
@ -40°C | ISO 180 | NB kJ/m2 |
Impact Resistance (Puncture), Energy @ Max. Loadh | | 2.5-mm Thick Plaques @ 23°C | ISO 6603-2 | 40 J |
2.5-mm Thick Plaques @ -40°C | ISO 6603-2 | 35 J |
3.2-mm Thick Plaques @ 23°C | ISO 6603-2 | 44 J |
3.2-mm Thick Plaques @ -40°C | ISO 6603-2 | 36 J |
Thermal Properties |
Deflection Temperature | |
@ 0.455 MPa (66 psi) | D 648 | 70 °C (158 °F) |
@ 1.82 MPa (264 psi) | D 648 | 64 °C (147 °F) |
Vicat Softening Temperature | D 1525 | 85 °C (185 °F) |
Thermal Conductivity | C 177 | 0.21 W/m·K (1.5 Btu·in./h·ft2·°F) |
Glass Transition Temperature (Tg) | DSC | 80 °C (176 °F) |
Specific Heat | | @ 100°C (212°F) | DSC | 1.76 kJ/kg·K (0.42 Btu/lb·°F) |
@ 150°C (302°F) | DSC | 1.88 kJ/kg·K (0.45 Btu/lb·°F) |
@ 200°C (392°F) | DSC | 1.97 kJ/kg·K (0.47 Btu/lb·°F) |
@ 250°C (482°F) | DSC | 2.05 kJ/kg·K (0.49 Btu/lb·°F) |
@ 60°C (140°F) | DSC | 1.30 kJ/kg·K (0.31 Btu/lb·°F) |
Coefficient of Linear Thermal Expansiond | D 696 | 5.1 x 10-5 /°C (mm/mm·°C) (2.8 x 10-5 /°F (in./in.·°F)) |
Typical Processing Conditions |
|
Mold Temperature | | 16-38 °C (60-100 °F) |
Processing Melt Temperature | | 249-271 °C (480-520 °F) |
Drying Time | | 4-6 hrs |
Drying Temperature | | 65 °C (150 °F) |
|