| Propertya | Test Methodb | Typical Value, Unitsc | 
|
| General Properties | 
|
| Specific Gravity | D 792 | 1.17 | 
| Injection Mold Shrinkage | D 955 | 0.005-0.007 mm/mm (0.005-0.007 in./in.) | 
| ISBM Blow Mold Shrinkagee | EMN | 0.012-0.016 mm/mm | 
| ISBM Bottle Properties | 
|
| Fill Volume Shrinkage - Boiling, 1 hrd | EMN | <1 % | 
| Fill Volume Shrinkage - Boiling, 2 hrd | EMN | <1.5 % | 
| Fill Volume Shrinkage - Dishwasherd | EMN | <1 % | 
| Microwave Steam Sterilization (Total Energy=Wattage*Minutes)d | EMN | Up to 11,200 W-min | 
| Microwave Boiling, Oven Powerd | EMN | Up to 2200 W | 
| Thermal Shock, Water Immersion, 98 C to 35 Cd | EMN | No effect | 
| Mechanical Properties (ISO Method) | 
|
| Tensile Strength @ Yield | ISO 527 | 45 MPa | 
| Tensile Strength @ Break | ISO 527 | 49 MPa | 
| Elongation @ Yield | ISO 527 | 7 % | 
| Elongation @ Break | ISO 527 | 130 % | 
| Tensile Modulus | ISO 527 | 1624 MPa | 
| Flexural Modulus | ISO 178 | 1531 MPa | 
Izod Impact Strength, Notched |  | | @ 23°C | ISO 180 | 66 kJ/m2 | 
| @ -40°C | ISO 180 | 14 kJ/m2 | 
| Mechanical Properties | 
|
| Tensile Stress @ Yield | D 638 | 44 MPa (6400 psi) | 
| Tensile Stress @ Break | D 638 | 53 MPa (7700 psi) | 
| Elongation @ Yield | D 638 | 7 % | 
| Elongation @ Break | D 638 | 140 % | 
| Tensile Modulus | D 638 | 1585 MPa (2.28 x 105 psi) | 
| Flexural Modulus | D 790 | 1585 MPa (2.28 x 105 psi) | 
| Flexural Yield Strength | D 790 | 66 MPa (9600 psi) | 
| Rockwell Hardness, R Scale | D 785 | 115 | 
Izod Impact Strength, Notched |  | | @ 23°C (73°F) | D 256 | 650 J/m (12.2 ft·lbf/in.) | 
| @ -40°C (-40°F) | D 256 | 126 J/m (2.4 ft·lbf/in.) | 
Impact Strength, Unnotched |  | | @ 23°C (73°F) | D 4812 | NB | 
| @ -40°C (-40°F) | D 4812 | NB | 
Impact Resistance (Puncture), Energy @ Max. Load |  | | @ 23°C (73°F) | D 3763 | 59 J (43 ft·lbf) | 
| @ -40°C (-40°F) | D 3763 | 63 J (46 ft·lbf) | 
| Optical Properties | 
|
| Total Transmittance | D 1003 | 92 % | 
| Haze | D 1003 | <1 % | 
| Properties After Boiling | 
| Haze |  | 
| After 8 hr boiling | EMN | <1 % | 
Izod Impact Strength, Notched, 23 C |  | | After 8 hr boiling | EMN | 650 J/m | 
| After re-equilibration |  | 643 J/m | 
Tensile Stress @ Yield |  | | After 8 hr boiling | EMN | 44 MPa | 
| After re-equilibration |  | 45 MPa | 
Elongation @ Yield |  | | After 8 hr boiling | EMN | 7 % | 
| After re-equilibration |  | 6.5 % | 
| Thermal Properties | 
| Deflection Temperature |  | 
| @ 0.455 MPa (66 psi) | D 648 | 109 °C (228 °F) | 
| @ 1.82 MPa (264 psi) | D 648 | 92 °C (198 °F) | 
| Typical Drying Conditions | 
|
| Drying Temperature |  | 88 °C (190 °F) | 
| Drying Time |  | 4-6 hrs | 
| Dewpoint |  | < -35 °C (< -30 °F) | 
| Typical Processing Conditions - Extrusion Blow Molding (EBM) | 
|
| Processing Melt Temperature |  | 240-250 °C (465-480 °F) | 
| Mold Temperature |  | 25-45 °C (80-110 °F) | 
| Typical Processing Conditions - Injection Molding | 
|
| Processing Melt Temperature |  | 260-282 °C (500-540 °F) | 
| Mold Temperature |  | 38-66 °C (100-150 °F) | 
| Typical Processing Conditions - Injection Stretch Blow Molding (ISBM) | 
|
| Processing Melt Temperature |  | 270-285 °C (520-545 °F) | 
| Injection Mold Temperature |  | 60-70 °C (140-160 °F) | 
| Preform Temperature at Blow |  | 185-195 °C (365-385 °F) | 
| Primary Blow Pressure |  | 0.03-0.08 MPa (4-12 psi) | 
| Secondary Blow Pressure |  | 0.2-0.3 MPa (25-40 psi) | 
| Blow Mold Temperature |  | 80-90 °C (175-195 °F) | 
| Residual Stress Under Polarized Light, Fringe Count | EMN | <= 3 | 
|  |